PLEXUS MA300/3000
Harmonization Code : 3904.61.00.00 | Polytetrafluoroethylene plates / sheets / film / tape / strip, self-adhesive, in rolls

Main features
- Simple 1:1 Meter-Mix Processing
- Fast 3-6 Minute Assembly
- High-Strength Stiff Cured Bond
Product Description
Plexus MA300 pairs a two-part, 1:1 methacrylate system with structural bonding of thermoplastics, metals, and composites. At 74 deg F (23 deg C), the non-sagging adhesive provides a 3-6 minute work time, reaches 500 psi (3.4 MPa) in 11-13 minutes, and reaches 1,000 psi (6.9 MPa) in 13-16 minutes. Typical cured tensile strength is 24.2-29.6 MPa with 20-40% elongation and 78 Shore D hardness. Applications include supported ABS, acrylic, FRP, gelcoat, PVC, steel, aluminum, polyester, styrenic, urethane, and vinyl-ester assemblies.
Key features
- Simple 1:1 Mixing: Uses equal component volumes for cartridge or meter-mix dispensing.
- 3-6 Minute Work Window: Supports rapid assembly at 74 deg F (23 deg C).
- 24.2-29.6 MPa Tensile Strength: Provides a high-strength cured methacrylate bond.
Applications
Applications include structural bonding of supported thermoplastics, metals, and composites, including ABS, acrylic, FRP, gelcoat, PVC, steel, aluminum, polyesters, styrenics, urethanes, and vinyl esters.
TDS, SDS & Technical Documents
Technical Specifications
General Properties
Physical Properties
Other Properties
Mechanical Properties
Additional Information
As-supplied / before-processing properties
Values are typical for the separate components and processing at 75 deg F (23.9 deg C) where stated.
| Property | Value | Unit | Method / condition |
|---|---|---|---|
| Component color - Part A / Part B | Beige / off-white | Typical uncured | |
| Mix ratio by volume | 1:1 | Part A to Part B | |
| Component density - Part A | 1.00 | g/mL | Typical uncured; +/- 0.02 |
| Component density - Part B | 0.96 | g/mL | Typical uncured; +/- 0.02 |
| Component viscosity - Part A / Part B | 40-70 / 40-70 | x 1,000 cP | Typical uncured |
| Work time | 3-6 | minutes | At 75 deg F (23.9 deg C) |
| Time to 500 psi (3.4 MPa) | 11-13 | minutes | At 75 deg F (23.9 deg C) |
| Shelf life | 13 | months | Recommended storage conditions |
After-processing / final-state properties
Values are typical cured properties; lap-shear results apply only to the stated substrate and test method.
| Property | Value | Unit | Method / condition |
|---|---|---|---|
| Gap tolerance | 0.25-3.2 | mm | Typical cured joint range |
| Hardness | 78 | Shore D | Typical cured property |
| Tensile strength | 24.2-29.6 | MPa | ASTM D638 / ISO 527 |
| Tensile modulus | 1,524-2,062 | MPa | ASTM D638 / ISO 527 |
| Elongation at break | 20-40 | % | ASTM D638 / ISO 527 |
| Lap shear - aluminum | 21.8 | MPa | ASTM D1002; adhesive failure |
| Lap shear - stainless steel | 23.1 | MPa | ASTM D1002; cohesive failure |